Inconel 718 vs A-286 Bolts: Which Superalloy Fastener for Your Application?
RAS Thermal Co., Ltd.
Applications
Alloy Identification and Standards
| Alloy | UNS No. | DIN / EN | Common ASTM/AMS fastener standards |
|---|---|---|---|
| Inconel 718 | N07718 | 2.4668 / NiCr19NbMo | ASTM B637, AMS 5662 / 5663 / 5664 |
| A-286 | S66286 | 1.4980 / X5NiCrTiMoVB25-15-2 | ASTM A453 Grade 660, AMS 5731 / 5732 / 5737 |
Chemical Composition, wt% (balance Fe)
The chemistry explains the cost gap. Inconel 718 carries 50-55 wt% nickel plus 4.75-5.50 wt% niobium, and the niobium forms the gamma-double-prime phase that gives the alloy its exceptional strength. A-286 holds nickel down to 24-27 wt% on an iron balance, relies on 1.90-2.35 wt% titanium for gamma-prime strengthening, and adds 0.001-0.010 wt% boron for grain-boundary control.
| Element | Inconel 718 UNS N07718 | A-286 UNS S66286 |
|---|---|---|
| Ni | 50.0-55.0 | 24.0-27.0 |
| Cr | 17.0-21.0 | 13.5-16.0 |
| Nb + Ta | 4.75-5.50 | - |
| Mo | 2.80-3.30 | 1.00-1.50 |
| Ti | 0.65-1.15 | 1.90-2.35 |
| Al | 0.20-0.80 | ≤0.35 |
| V | - | 0.10-0.50 |
| Co | ≤1.0 | - |
| C | ≤0.08 | ≤0.08 |
| Mn | ≤0.35 | ≤2.00 |
| Si | ≤0.35 | ≤1.00 |
| P | ≤0.015 | ≤0.025 |
| S | ≤0.015 | ≤0.025 |
| B | ≤0.006 | 0.001-0.010 |
Minimum Room-Temperature Mechanical Properties
| Property | Inconel 718 | A-286 |
|---|---|---|
| Condition | Solution annealed + aged | Solution treated + aged |
| Tensile strength, ksi / MPa | 185 / 1275 | 130 / 895 |
| Yield strength, 0.2% offset, ksi / MPa | 150 / 1034 | 85 / 586 |
| Elongation, % | 12 | 15 |
| Hardness, HB | 331-444 | 248-341 |
| Typical continuous service limit | 1300°F / 704°C | 1200°F / 649°C |
What Is the Strength Difference in Practice?
On the numbers, Inconel 718 delivers about 42% higher minimum tensile strength than A-286 (1275 MPa against 895 MPa) and roughly 76% higher minimum yield strength (1034 MPa against 586 MPa). That margin is what qualifies 718 for fatigue-critical rotating hardware and high-preload structural joints. The trade is material cost: with 50-55 wt% nickel against A-286’s 24-27 wt%, the 718 fastener blank costs meaningfully more per piece before heat treatment even enters the picture.
Application Notes
Inconel 718 (UNS N07718)
Inconel 718 is a precipitation-hardened nickel-chromium alloy used for high-strength bolting in gas turbines, oil and gas, nuclear, and cryogenic service. It offers high creep-rupture strength and oxidation resistance to 1300°F (704°C) under load, and is NACE MR0175 / ISO 15156 sour-service qualified in the aged condition. Select it when tensile/yield above 160 ksi / 120 ksi is required, or when chloride SCC and sour corrosion resistance are critical.
A-286 (UNS S66286)
A-286 is a precipitation-hardened iron-nickel austenitic alloy used for moderate-temperature fasteners, turbine frames, afterburners, and automotive turbocharger bolting. It offers good oxidation resistance to 1500°F (816°C) intermittent, at a lower raw-material cost than Inconel 718 because of its lower nickel content. Select it when 85-100 ksi yield strength is sufficient, service temperature stays below 1200°F (649°C), or cost is a primary driver.
How to Select the Right Bolt Grade
- Confirm the temperature ceiling. Above 649°C continuous, A-286 drops out of the running. Inconel 718 holds design allowables to 704°C.
- Check the strength requirement. If 85-100 ksi yield meets the joint design, A-286 suffices, at 120 ksi yield and above, move to 718.
- Check the environment. Sour (H2S) exposure or chloride SCC risk points to 718 in the aged, NACE MR0175-qualified condition.
- Compare total fastener cost. Where both grades meet the specification, A-286’s lower nickel content usually makes it the cheaper bolt by a clear margin.
Standards and External References
Inconel 718 fasteners are governed by ASTM B637 and AMS 5662/5663/5664. A-286 fasteners by ASTM A453 Grade 660 and AMS 5731/5732/5737. For the underlying specifications, see ASTM International and SAE International.
Frequently Asked Questions (FAQ)
What is the main difference between Inconel 718 and A-286 bolts?
Strength and cost. Inconel 718 delivers 185 ksi (1275 MPa) minimum tensile and 150 ksi (1034 MPa) yield, versus 130 ksi (895 MPa) tensile and 85 ksi (586 MPa) yield for A-286. A-286 carries roughly half the nickel content (24-27 wt% versus 50-55 wt%), which makes it the lower-cost fastener grade.
What are the temperature limits for each alloy?
Inconel 718 is typically limited to 704°C (1300°F) continuous service under load. A-286 is limited to about 649°C (1200°F) continuous, with good intermittent oxidation resistance to 816°C (1500°F).
When should I choose A-286 instead of Inconel 718?
Choose A-286 when service stays below 649°C, yield strength requirements of 85-100 ksi are sufficient, and cost is a primary driver. Typical uses include turbine frames, afterburners and automotive turbocharger bolting.
Is Inconel 718 suitable for sour (H2S) service?
Yes. In the aged condition Inconel 718 is qualified to NACE MR0175 / ISO 15156 for sour oil and gas service, which is why it is common in wellhead and downhole bolting.
Need material for your application?
Tell us the grade, form, dimensions and quantity. We'll get you a quote with a sample MTC within 24 hours.
Request a Quote