AMS 5662 is the SAE aerospace material specification for Alloy 718 bar, forgings and rings: 52.5Ni-19Cr-3.0Mo-5.1Cb-0.90Ti-0.50Al-18Fe, consumable-electrode or vacuum-induction melted, solution heat treated and precipitation hardenable. On this site, Inconel 718 (UNS N07718) is Anchored against AMS 5662 / 5663 and ASTM B637 for its bar and forging forms. AMS 5662 is the document behind “bar per AMS 5662”. It is not a different alloy from ASTM B637. It is the aerospace-controlled version of the same chemistry, with tighter trace elements, defined melt practice and a specified heat-treatment cycle.
What AMS 5662 covers
| Item | Scope |
|---|---|
| Product forms | Bar, forgings, forging stock and rings |
| Alloy | 52.5Ni-19Cr-3.0Mo-5.1Cb-0.90Ti-0.50Al-18Fe (Alloy 718 / UNS N07718) |
| Condition | Solution heat treated at 1775 °F (968 °C), precipitation hardenable |
| Melt practice | Consumable-electrode (VAR) or vacuum-induction (VIM) melted |
| Companion specs | AMS 5663 / 5664 (bar, forgings, rings variants) · AMS 5596 / 5597 (sheet, strip, plate) |
Where a drawing says “bar per AMS 5662”, the mill certificate must cite AMS 5662 and the heat must be reported against its chemistry and condition, not merely against a nominal “718” chemistry.
The chemistry window behind the AMS number
The AMS 5662 window is the γ″-forming composition that makes 718 age-hardenable:
| Element | Range (wt %) |
|---|---|
| Ni | 50.0-55.0 |
| Cr | 17.0-21.0 |
| Nb (+Ta) | 4.75-5.50 |
| Mo | 2.80-3.30 |
| Ti | 0.65-1.15 |
| Al | 0.20-0.80 |
| Fe | Balance |
| C | ≤ 0.08 |
The niobium content is the load-bearing figure: it forms the coherent Ni₃Nb (γ″) precipitate that produces the strength increase on ageing. Too little niobium and the mechanical targets are missed, too much promotes Laves or δ phase and reduces ductility. Aerospace heats also tighten phosphorus, sulfur and gas limits, so a heat that passes a general chemistry check can still fail an AMS cleanliness requirement.
AMS 5662 versus ASTM B637 versus AMS 5663
All three describe 718 bar, but they are used for different reasons:
| Specification | Use |
|---|---|
| ASTM B637 | The general ASTM material specification for precipitation-hardening nickel bar and forgings, the industrial baseline |
| AMS 5662 | The aerospace AMS specification for 718 bar, forgings and rings, tighter control, defined melt and heat treat |
| AMS 5663 | A companion AMS 718 specification used where a different condition or inspection package applies |
In practice, a project drawing usually names the AMS number when the part flies and the ASTM number when the part is industrial, quoting an AMS heat against a B637 requirement is over-specification, and quoting a B637 heat against an AMS 5662 requirement is non-conformance.
Mechanical basis and how to order
The verified 718 design data on this site, in the solution + aged condition:
| Condition | UTS | Yield (0.2 %) | Elongation | Hardness |
|---|---|---|---|---|
| Room temperature | 1275 MPa | 1035 MPa | 12% | 38 HRC |
| 650 °C | 860 MPa | 795 MPa | 18% | n/a |
To order, state: Alloy 718, UNS N07718, bar per AMS 5662, the diameter and length, the condition (solution + aged), the acceptance (tensile at room and 650 °C, stress-rupture where applicable) and the certificate (EN 10204 3.1 with heat-specific chemistry; 3.2 witnessed where required). Use the RFQ spec writer to assemble it, and the weight calculator for the bar weight.
How to select the right option for your process
Work through these checks in order so the component stays inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
What does AMS 5662 cover?
It is the SAE aerospace specification for Alloy 718 (UNS N07718) bar, forgings, forging stock and rings, 52.5Ni-19Cr-3.0Mo-5.1Cb-0.90Ti-0.50Al-18Fe, consumable-electrode or vacuum-induction melted, solution heat treated and precipitation hardenable.
Is AMS 5662 the same as Inconel 718?
It is the aerospace specification for the same alloy, Alloy 718 / UNS N07718. The alloy is identical; AMS 5662 adds controlled melt practice, tighter trace-element limits and a defined heat-treatment cycle.
AMS 5662 or ASTM B637 for 718 bar?
Use AMS 5662 when the drawing calls for aerospace-grade bar, forgings or rings; use ASTM B637 for the industrial baseline. They cover the same chemistry and condition, with AMS adding the aerospace control and documentation package.
What is the niobium range in AMS 5662?
Niobium (plus tantalum) is 4.75-5.50 wt %. It is the critical figure because it forms the γ″ (Ni₃Nb) precipitate that gives 718 its age-hardened strength.