A certificate is not a grade label. It is evidence that a specific heat meets a named standard. Which evidence is required, and how strong it has to be, depends on the grade and the duty: an OES chemistry report proves a corrosion grade, an aged hardness and stress-rupture record proves a turbine grade, and a certified grain size proves a creep grade. This page sets out the two certificate levels, the test lines that carry the proof for each family, and the overlays that escalate the requirement for sour service and aerospace hardware.
EN 10204 3.1 vs 3.2, what each level actually proves
| Level | Who signs | What it evidences |
|---|---|---|
| EN 10204 3.1 | The manufacturer’s authorised inspection representative | Inspection results from the specific heat you receive, chemistry and mechanicals, against the specified standard |
| EN 10204 3.2 | The manufacturer together with an independent third party | The same heat-specific evidence, but the testing has been witnessed and countersigned by a party with no commercial interest in the result |
The difference is who witnessed it, not what was tested. 3.1 already proves the heat; 3.2 removes the manufacturer’s sole signature from the chain. Neither level is a “grade certificate” that covers a whole product family, both are tied to a heat and a standard, which is why an unscoped certificate is worth nothing on an audit.
The chemistry line: OES against the standard’s window
Every grade is proven first by chemistry, and the evidence is OES or spark analysis of the heat, reported element by element against the window in the governing standard. The elements that matter are the ones the grade’s job depends on, and knowing them tells you what to look for on the report:
- Ni-Cr-Mo corrosion grades: C-276 against C-22 turns on the chromium and molybdenum ratio and the carbon limit (the low-carbon ceiling is what protects the weld zone). C-276’s molybdenum and tungsten carry the reducing-acid resistance.
- 718 (N07718): the niobium window is the tightest line, with titanium and aluminium beside it, because the γ″ strengthening depends on all three.
- Precision and expansion grades: the chemistry is proven so that the physical property (expansion, permeability) can be attributed to a known composition.
A certificate that reports chemistry without naming the standard’s window cannot be reconciled, and one that reports the elements without a heat number cannot be traced.
The mechanical line: tension, hardness and grain size
The mechanical evidence is tied to the grade’s specified acceptance:
- Tension per ASTM E8/E8M (the tension-testing method this site anchors), tensile, yield and elongation at the condition supplied.
- Hardness where the grade is bought by condition: Inconel 718 aged to 38 HRC, Hastelloy C-276 at 90 HRB in the annealed state, both verified values that the certificate has to reproduce.
- Grain size where grain structure is the property: Incoloy 800H is supplied solution annealed to ASTM grain size 5 or coarser, and that is a certified creep-strength feature, not a cosmetic note. A fine-grained heat is a different material for the duty.
For forgings and bar, the test coupons must be taken as the standard requires and identified to the heat, an unlinked coupon result is not evidence for the part.
Service-qualification overlays
Beyond the mill grade, some duties add a qualification layer:
| Overlay | Applies to | What it adds |
|---|---|---|
| NACE MR0175 / ISO 15156 | C-276, Inconel 625, Monel 400 in sour (H₂S) service | A service qualification on top of the mill grade, hardness and chemistry limits for sour exposure |
| AMS rotating-quality packages | Inconel 718, Waspaloy | Trace-element limits, defined melt practice and inspection for flight-critical rotating parts |
| ASTM F / MIL specifications | MP35N, L605, 4J29 | Implant-grade cleanliness, or sealing-alloy leak and expansion criteria |
An overlay is not a grade: NACE MR0175 does not make a material a C-276, and an AMS package does not change the alloy. Each one narrows what the same alloy must prove on top.
Grade-by-grade matrix
The governing standards below are the verified site callouts for each stocked grade, the documents a certificate should cite:
| Grade | UNS / GB | Governing standards (verified) | Verified ceiling |
|---|---|---|---|
| Inconel 718 | N07718 | AMS 5662 · AMS 5663 · ASTM B637 · UNS N07718 | 650 °C |
| Inconel 625 | N06625 | ASTM B443 · ASTM B444 · ASTM B446 · AMS 5666 · NACE MR0175 | 980 °C |
| Hastelloy C-276 | N10276 | ASTM B575 · ASTM B574 · ASTM B564 · UNS N10276 | 400 °C |
| Hastelloy X | N06002 | AMS 5536 · AMS 5754 · ASTM B435 · ASTM B572 | 1100 °C |
| Monel 400 | N04400 | ASTM B164 · ASTM B127 · ASTM B165 · NACE MR0175 | 540 °C |
| Nimonic 80A | N07080 | ASTM B637 · BS HR 201 · AMS 5763 · DIN 17742 | 815 °C |
| Waspaloy | N07001 | AMS 5708 · AMS 5709 · AMS 5544 · ASTM B637 | 870 °C |
| Nickel 200 | N02200 | ASTM B160 · ASTM B161 · ASTM B162 · ASME SB-160 | 315 °C |
| MP35N | R30035 | ASTM F562 · AMS 5844 · AMS 5845 · ISO 5832-6 | 425 °C |
| L605 | R30605 | AMS 5759 · AMS 5537 · ASTM F90 | 980 °C |
| 4J29 | n/a | ASTM F15 · GB/T 14986 · MIL-I-23011 | 450 °C |
| 4J36 | n/a | ASTM F1684 · GB/T 14986 · AFNOR NF A54-301 | 230 °C |
| 1J22 | n/a | GB/T 14986 · AMS 7717 equivalent · ASTM A801 | 450 °C |
| 1J50 | n/a | GB/T 14986 · IEC 60404-8-6 | 450 °C |
| Incoloy 800 | N08800 | ASTM B163 · ASTM B407 · ASTM B408 · ASME SB-407 | 1100 °C |
| Incoloy 800H | N08810 | ASTM B163 · ASTM B407 · ASME SB-163 · ASME Section III/VIII | 1100 °C |
| Incoloy 800HT | N08811 | ASTM B163 · ASTM B407 · ASME SB-163 · NACE MR0175 | 1100 °C |
| Incoloy 825 | N08825 | ASTM B163 · ASTM B423 · ASTM B424 · NACE MR0175 | 540 °C |
| Incoloy 925 | N09925 | ASTM B805 · NACE MR0175 · API 6A | 650 °C |
| 3J21 | n/a | GB/T 14986 · YB/T 5253 | 350 °C |
Read the table as a form warning as well as a standards list: several grades appear under more than one document because the form decides which one applies, AMS 5662 for 718 bar against AMS 5596 for 718 plate, B575 for C-276 plate against B574 for C-276 bar. A certificate that cites the wrong form standard for the product delivered is a non-conformance even when the chemistry is correct.
How to audit a certificate in six lines
When the paperwork arrives, six checks settle it:
- Heat number: present, and identical to the marking on the goods.
- Standard: named, and the form-specific one for this product (not a sibling specification).
- Chemistry: element-by-element results reconciled to that standard’s window, with the discriminating elements visible.
- Mechanicals: tested at the supplied condition, with hardness or grain size where the grade specifies it.
- Certificate level: EN 10204 3.1 signed by the manufacturer’s inspection representative, or 3.2 with the independent party named.
- Overlays: NACE MR0175 or the AMS package cited where the duty requires it.
Six lines, six rejections avoided, which is why the specification should be written to make each of them checkable before the order is placed.
How to select the right option for your process
Five checks, in order. Each one keeps the component inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
What is the difference between EN 10204 3.1 and 3.2?
Both prove the specific heat against a named standard with chemistry and mechanical results. 3.1 is signed by the manufacturer’s authorised inspection representative; 3.2 adds an independent third party who witnesses the testing and countersigns. The difference is who witnessed the tests, not what was tested, and neither replaces the need to cite the correct standard for the product form.
Why does the certificate have to cite a form-specific standard?
Because the product form changes the requirements: AMS 5662 covers 718 bar, forgings and rings, while AMS 5596 covers sheet, strip and plate; ASTM B575 covers C-276 plate where B574 covers bar. A certificate that cites the wrong form standard does not cover the product you received, even when the alloy chemistry is correct.
Which grades need a grain-size result on the certificate?
Incoloy 800H is the clear case: it is supplied solution annealed to ASTM grain size 5 or coarser, and that coarse grain is the creep-strength feature the grade is bought for. A fine-grained heat does not deliver the intended behaviour, so the grain size belongs on the certificate rather than in a datasheet.
What is an AMS rotating-quality package?
For grades such as Inconel 718 and Waspaloy, the aerospace AMS specifications layer on tighter trace-element limits, defined melt practice and inspection for flight-critical rotating parts, on top of the chemistry and mechanical lines. It is a qualification overlay on the same alloy, not a separate grade.