Inconel 718 gets its design strength from the furnace, not just the mill. The verified site data, 1275 MPa UTS and 1035 MPa yield at 38 HRC: only exists in the fully precipitation-hardened condition, and that condition is reached by a specific double-age cycle written into AMS 5662 / AMS 5663. Skip or mistime the cycle and the same UNS N07718 chemistry delivers a fraction of the strength: the γ″ (Ni₃Nb) strengthening phase has to be dissolved, then re-precipitated at two controlled temperatures with a controlled cooling ramp between them.
The AMS 5662 cycle, step by step
The route below is the standard aerospace cycle for Alloy 718 bar and forgings, cross-checked across the Special Metals technical bulletin, the Carpenter alloy-718 processing sheet (AMS 5662N §3.4 / §3.5.1.2) and the Aircraft Materials condition table:
| Step | Condition | Note |
|---|---|---|
| 1. Solution treat | 954-968 °C, about 1 h, air cool | AMS window 941-1,010 °C (1,725-1,850 °F); 968 °C (1,775 °F) is the figure cited on the AMS 5662 scope |
| 2. First age | 718 °C / 8 h | 1,325 °F, precipitates the fine γ″ |
| 3. Controlled cool | furnace cool at ~55 °C/h down to 621 °C | the ramp is part of the specification, not a courtesy |
| 4. Second age | 621 °C / ≥8 h, air cool | 1,150 °F, completes the double-age sequence to a total ageing time of about 18 h |
After step 4 the verified design numbers apply: 1275 MPa UTS, 1035 MPa yield, 12% elongation, 38 HRC hardness at room temperature.
Why the double age and the slow ramp
The two-stage age is what balances strength against notch ductility. At 718 °C the γ″ (Ni₃Nb) precipitate nucleates densely, the slow 55 °C/h ramp and the 621 °C hold let the precipitate coarsen just enough that the matrix is not over-strengthened into a notch-brittle state. A single-stage age can hit the hardness figure while missing the stress-rupture and notch-ductility targets, which is why the certificate must record both temperatures and both hold times, not a summary condition name. The alternative route pair exists for a reason: AMS 5664 / 5597 substitute a 1,038-1,950 °F solution treatment for creep-rupture-limited hot-section parts, trading some room-temperature tensile for transverse ductility and rupture life.
Where the cycle belongs on the paperwork
Order it in three layers: (1) the grade and UNS, Alloy 718 / UNS N07718; (2) the governing document and condition, bar per AMS 5662, solution treated (ageing by the buyer) or per AMS 5663, solution treated and precipitation heat treated (delivered aged); (3) the acceptance, room-temperature tensile per ASTM E8, hardness after ageing, and stress-rupture at 650 °C where the duty is creep-critical. Require the EN 10204 3.1 certificate to carry the recorded solution and ageing temperatures with hold times, so the route is auditable. The RFQ spec writer assembles the field list, and the heat-treatment hub puts this cycle in the wider solid-solution vs precipitation-hardened context.
How to select the right option for your process
Five checks, in order. Each one keeps the component inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
What is the standard heat treatment for Inconel 718?
The AMS 5662 cycle: solution treat at 954-968 °C for about 1 hour and air cool; age at 718 °C for 8 hours; furnace cool at roughly 55 °C/h to 621 °C; hold at 621 °C for at least 8 more hours (about 18 hours total ageing); then air cool. The verified result is 38 HRC with 1275 MPa UTS.
AMS 5662 or AMS 5663 for the same bar?
They differ in delivery condition, not chemistry. AMS 5662 bar arrives solution treated and is aged by the buyer after machining; AMS 5663 bar arrives already solution treated and precipitation heat treated at full design strength. Buy 5662 when heavy machining precedes ageing, and 5663 when the part is finished and delivered at strength.
Can Inconel 718 be machined after ageing?
Light finishing only. The aged condition at 38 HRC and 1035 MPa yield work-hardens aggressively and cuts slowly; roughing belongs in the solution-treated condition, with the double-age cycle run after the heavy stock removal. Major machining after ageing risks tool chipping and residual stress.
Does welding 718 need a post-weld heat treatment?
Yes, where design strength matters: weld in the solution-treated condition with the matching ERNiFeCr-2 filler, then run the full solution-plus-double-age cycle so the weld metal and HAZ reach the design properties. The slow γ″ kinetics are what make 718 weldable without strain-age cracking in the first place.