Incoloy 800 series tube and bar stock
Selection Guide / Incoloy 800

Incoloy 800H vs 800HT

Two grades that look identical on a datasheet, differ in the hundredths of a percent, and part company at 900 °C. Here is exactly where, and why.

The short answer

§01, Summary

Below 900 °C

Effectively the same grade

Same nickel, chromium, iron, density and melting range. Substituting one for the other at moderate temperature is common practice and rarely matters.

Above 900 °C

800HT earns its premium

Higher carbon floor plus tighter Al and Ti holds the combined content up, which buys creep-rupture strength in reformer and furnace duty.

On the certificate

N08810 vs N08811

Different UNS numbers. If the certificate does not cite N08811 with Al and Ti individually, it has not established 800HT.

Line by line

§02, Specification

Both grades are quoted to ASTM B407 for bar and B409 for plate. Everything below is the specification range; the last column is where the two actually diverge.

Item 800H (N08810) 800HT (N08811) Difference
UNS N08810 N08811 Different UNS numbers — not interchangeable on a certificate
Governing spec ASTM B407 (bar) / B409 (plate) ASTM B407 (bar) / B409 (plate) Same documents, different grade line
Nickel 30.0–35.0 30.0–35.0 Identical
Chromium 19.0–23.0 19.0–23.0 Identical
Carbon 0.05–0.10 0.06–0.10 HT raises the carbon floor
Aluminium 0.25–0.75 0.25–0.60 HT narrows the window
Titanium 0.25–0.75 0.25–0.60 HT narrows the window
Al + Ti combined Nominally lower Constrained near the top of the window The real discriminator
Iron Balance Balance Identical
Density 7.94 g/cm³ 7.94 g/cm³ Identical
Melting range 1350–1400 °C 1350–1400 °C Identical
Max service temp 1100 °C 1100 °C Same ceiling, different strength above 900 °C

Composition basis: ASTM B407 / B409. Both grades are supplied to a coarse-grain condition; the anneal is part of the specification, not a mill preference.

Why 0.01% of carbon buys a separate grade

§03, Mechanism

Carbon sets the creep resistance

Carbon in solid solution and as fine carbides pins grain boundaries and slows the deformation that kills a part at temperature. Raising the floor from 0.05 to 0.06 wt% is small in absolute terms but it shifts the distribution upward across a whole heat.

Al and Ti form the strengthening particles

Aluminium and titanium combine with nickel to form gamma-prime precipitates. Narrowing their windows to 0.25–0.60 each keeps the combined content in a band that produces a useful amount of precipitate without destabilising the austenite.

The anneal locks it in

Coarse grain is the point of the heat treatment: fewer grain boundaries means slower creep. That is why the certificate should state the anneal temperature and the grain size — chemistry alone does not deliver the property.

Five duties, five answers

§04, Decision

Reformer tube or pigtail, loaded, 950 °C

→ 800HT

This is the duty the grade exists for. The creep-rupture advantage at temperature is the entire purchase decision, and 800H at the same wall thickness will deform earlier.

Furnace roller, 850 °C, moderate load

→ Either

Below roughly 900 °C the two are close enough that availability and price can decide. Document the substitution if your customer's specification names one grade.

Heat exchanger tubing, 600 °C, corrosive process

→ Either

Corrosion resistance is essentially identical; the choice is a procurement question rather than a metallurgical one.

Existing 800H part failing by sag at 930 °C

→ 800HT, with a section check

Upgrading the grade is the first move, but verify the wall thickness against the higher-temperature creep data before assuming the same geometry survives.

Spare-part order from an old drawing that names 800H

→ 800H as drawn

Do not silently substitute. If 800HT is offered as an alternative, state it as a deviation and let the drawing owner accept it in writing.

Three lines to check on the MTC

§05, Certificate

01

UNS number. N08810 or N08811. Not "800 series", not "Alloy 800".

02

Carbon, aluminium and titanium individually. Al and Ti must be separate so the combined content can be checked.

03

Anneal temperature and grain size. The property comes from the heat treatment; without these two lines the chemistry is not enough.

Eight questions buyers ask

§06, Questions

What is the actual difference between Incoloy 800H and 800HT?

Carbon and the aluminium-titanium balance, plus the annealing temperature that goes with them. 800HT raises the carbon floor from 0.05 to 0.06 wt% and narrows aluminium and titanium to 0.25–0.60 each, which holds the combined Al+Ti content up near the top of the window. That tighter chemistry, with the higher solution-anneal temperature the specification requires, is what buys additional creep-rupture strength above roughly 900 °C.

Are 800H and 800HT interchangeable?

Below about 900 °C, in practice yes for most duties, and many buyers substitute one for the other without consequence. Above 900 °C they are not equivalent: 800HT's higher and tighter Al+Ti content gives it measurable creep-rupture advantage, which is the only reason the grade exists. If your part operates above 900 °C under load, the substitution needs a creep calculation, not a judgement call.

Why does the density not change if the chemistry changes?

Because the differences are in the hundredths of a percent. Carbon moves by 0.01 wt%, and aluminium and titanium shift within a window that is a fraction of a percent of the total mass. Density stays at 7.94 g/cm³ for both, so the same drawing weighs the same in either grade — your costing does not change, only the metallurgy does.

Does 800HT cost more than 800H?

Slightly, and the gap is small compared with the alloy families above it. The premium is not metal content — both contain 30–35% nickel and 19–23% chromium — it is the tighter chemistry control and the higher annealing temperature. Both grades also require a coarse-grain condition, which is a heat-treatment discipline rather than an ingredient.

What does the mill certificate need to show for 800HT?

The UNS number N08811, the carbon content, and the aluminium and titanium contents individually so the combined Al+Ti can be checked. It should also state the solution-anneal temperature and the grain size, because the creep properties depend on the heat treatment and not only on chemistry. A certificate that lists only nickel, chromium and iron does not establish that the material is 800HT rather than 800H.

Can I use 800H instead of 800HT to save cost on a furnace part?

Yes if the service temperature is comfortably below 900 °C, and it is a legitimate saving. No if the part is a reformer tube, a pigtail or a furnace roller that carries load at 950 °C and above — that is precisely the duty the HT variant was created for, and the cost saving will be repaid as premature deformation.

Which one welds more easily?

They weld the same way; the difference is in what the procedure has to say afterwards. Both are austenitic and neither is age-hardened, so no post-weld ageing is involved. For thick-section or restrained welds, the filler selection and the heat input matter more than the choice between these two grades.

How do I write the order so I get the grade I asked for?

State the grade with the UNS number and the product-form standard: for example 'Incoloy 800HT, UNS N08811, ASTM B407, annealed, 25 mm bar'. Add the service temperature and whether the part carries load at temperature. That last sentence is what distinguishes an 800H order from an 800HT order in the supplier's eyes.

Full grade data

§07, Datasheets

Tell us the temperature and the load

That is what decides between 800H and 800HT. The quote will name the UNS number, the anneal and the certificate level, so the grade you receive is the grade you specified.

Ask for an 800H / 800HT recommendation
Request a Quote
Add RAS Thermal as a preferred source on Google