AMS 5663 is the Alloy 718 bar, forging and ring specification where the seller runs the furnace: solution treated and precipitation heat treated at delivery, with 185 ksi (1,276 MPa) UTS, 150 ksi (1,034 MPa) yield and 12 % elongation minimums to prove on the mill certificate. AMS 5662 covers the same UNS N07718 chemistry in the solution-treated-only condition, the buyer ages it later. The two numbers name two different points in the same thermal route, and choosing between them is a manufacturing-sequencing decision, not an alloy decision.
5662 vs 5663 vs 5664, same alloy, three delivery states
| Specification | Delivery condition | What the buyer receives |
|---|---|---|
| AMS 5662 | solution treated (~954-968 °C), precipitation hardenable | soft stock at ≤ 277 HB for heavy machining, the double-age cycle happens later, at the buyer |
| AMS 5663 | solution treated + precipitation heat treated | the finished-condition bar: 185 ksi / 150 ksi / 12 % at ≥ 331 HB, verified on the certificate |
| AMS 5664 | higher-temperature solution (1,900-1,950 °F) variant | creep-rupture-oriented hot-section stock |
The condition split is visible in the SAE titles themselves: 5662 ends “solution treated”, 5663 ends “solution treated and precipitation heat treated”. Same γ″ chemistry (Ni 50-55, Cr 17-21, Nb+Ta 4.75-5.50, Mo 2.80-3.30 %), two different furnaces doing the last step.
The cycle behind the 185 ksi floor
AMS 5663 material is the product of the standard double-age route: solution at 954-968 °C with air cool, first age at 718 °C / 8 h, furnace cool at ~55 °C/h to 621 °C, second age at 621 °C / ≥8 h, air cool. Run on the verified site chemistry, that route produces 1275 MPa UTS / 1035 MPa yield / 12% elongation at 38 HRC: the same condition the 5663 floors describe in imperial units. Buying 5663 moves the furnace responsibility to the mill: the certificate must carry the actual solution and ageing temperatures with hold times, hardness in the aged band, and tensile per ASTM E8, the audit trail the buyer’s own furnace would otherwise own. See the cycle detail for the step table.
Ordering rules and where 5663 fits
Order 5663 when the part ships at full design strength: final machined components delivered to assembly, rotating hardware where the OEM signs off the aged condition, and repair shops replacing aged hardware without a furnace on site. Order 5662 when heavy machining precedes ageing and the buyer’s heat treatment is part of the routing. State: Alloy 718, UNS N07718, bar per AMS 5663, size, the aged-condition acceptance (185/150/12 min, hardness ≥ 331 HB), VIM + VAR melt where the drawing calls it, and EN 10204 3.1 with the recorded thermal route. The RFQ spec writer formats the lines, the equivalent-grades page shows where GH4169 / 2.4668 cross-references sit against the AMS set.
How to select the right option for your process
Five checks, in order. Each one keeps the component inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
What is AMS 5663?
The SAE aerospace specification for Alloy 718 (UNS N07718) bar, forgings, forging stock and rings delivered solution treated AND precipitation heat treated, with 185 ksi UTS, 150 ksi yield and 12 % elongation minimums verified on the mill certificate in the aged condition.
AMS 5662 or 5663, which should I buy?
Buy 5662 when your shop machines heavily and runs the ageing itself after roughing; buy 5663 when the material must arrive at full aged strength with the furnace work already certified. The chemistry is identical; the delivery condition is the whole difference.
What hardness is AMS 5663 bar?
The aged condition verifies at ≥ 331 HB, corresponding to the 38 HRC class of the fully aged site-verified data (1275 MPa UTS / 1035 MPa yield). Solution-treated 5662 stock, by contrast, stays at or below 277 HB for machinability.
Is AMS 5663 the same as ASTM B637?
B637 is the ASTM precipitation-hardening bar and forging document the industrial side cites; AMS 5663 is the aerospace-controlled SAE version with defined melt practice and the aged delivery condition. Aerospace drawings call 5663; general industrial bar usually cites B637. They are not interchangeable acceptance documents.