AMS 5596 is the SAE aerospace material specification for Alloy 718 sheet, strip and plate: the flat-product counterpart to AMS 5662 (bar, forgings, rings). Both describe the same UNS N07718 chemistry, they differ by product form. On this site, Inconel 718 is available as Plate and Strip (as well as bar, wire, spring wire and forging), and its datasheet anchors AMS 5662 / 5663 for bar together with ASTM B637. When a drawing calls “plate per AMS 5596”, it is AMS 5596, not AMS 5662, that the mill certificate must cite, because the flat-product requirements (grain, surface, flatness, mechanical sampling) are specified per form.
What AMS 5596 covers
| Item | Scope |
|---|---|
| Product forms | Sheet, strip and plate |
| Alloy | 52.5Ni-19Cr-3.0Mo-5.1Cb-0.90Ti-0.50Al-18Fe (Alloy 718 / UNS N07718) |
| Condition | Solution heat treated at 1775 °F (968 °C), precipitation hardenable |
| Companion specs | AMS 5597 (sheet, strip, plate variant) · AMS 5662 / 5663 / 5664 (bar, forgings, rings) |
| ASTM counterpart | ASTM B670 (718 plate, sheet and strip) |
The pairing to remember: AMS 5596 for flat product, AMS 5662 for long product. Quoting bar under a plate requirement, or vice versa, is a non-conformance even though the alloy is the same.
Chemistry and condition
AMS 5596 holds the same γ″-forming composition as the bar specification:
| Element | Range (wt %) |
|---|---|
| Ni | 50.0-55.0 |
| Cr | 17.0-21.0 |
| Nb (+Ta) | 4.75-5.50 |
| Mo | 2.80-3.30 |
| Ti | 0.65-1.15 |
| Al | 0.20-0.80 |
| Fe | Balance |
| C | ≤ 0.08 |
The material is supplied solution heat treated and is precipitation hardenable: the part is aged (double aged) after forming, which is why flat product is bought in the solution-treated condition and hardened in the fabrication route. Strength follows the condition, not the form: the verified 718 design values are 1275 MPa UTS / 1035 MPa yield at room temperature in the aged condition.
Why form-specific AMS matters for plate
Plate and sheet carry requirements a bar specification does not: thickness tolerance and flatness, surface finish, sampling location, and for some applications grain size. A mill that certifies 718 bar to AMS 5662 has certified a long product to a long-product specification, that certificate does not cover a plate. Where the design cites AMS 5596, require the certificate to cite AMS 5596 and the plate dimensions, with the mechanical tests sampled per that specification.
How to order 718 plate
State: Alloy 718, UNS N07718, plate per AMS 5596 (or ASTM B670 for the industrial equivalent), the thickness, width and length, the condition (solution heat treated, state whether aged is required), the acceptance tests and the certificate (EN 10204 3.1 heat chemistry, or 3.2 witnessed). Compute the plate weight from the verified 8.19 g/cm³ density, a square metre at t mm weighs 81.9 kg at 10 mm, with the weight calculator by grade and form, and see the Inconel 718 price per kg page for the indicative band.
How to select the right option for your process
Work through these checks in order so the component stays inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
What does AMS 5596 cover?
It is the SAE aerospace specification for Alloy 718 (UNS N07718) sheet, strip and plate, the flat-product counterpart to AMS 5662, which covers bar, forgings and rings. Same chemistry, different product form.
AMS 5596 or AMS 5662 for 718 plate?
AMS 5596. It is the flat-product specification. AMS 5662 applies to bar, forgings and rings. The alloy is identical but the certificate must cite the specification that matches the form.
What is the ASTM counterpart to AMS 5596?
ASTM B670, which covers precipitation-hardening nickel alloy plate, sheet and strip. Use AMS 5596 for aerospace and ASTM B670 for the industrial equivalent.
Is 718 plate supplied aged or solution treated?
Flat product is normally supplied solution heat treated and is precipitation hardenable; the ageing (double ageing) is applied after forming in the fabrication route. State the condition required on the purchase order.