AMS 5597 covers Alloy 718 (UNS N07718) sheet, strip and plate in the solution-treated-at-1,950 °F (1,066 °C) condition, the high end of the 718 solution window, roughly 100 °F above the AMS 5596 ceiling. Same γ″ chemistry as every 718 document (Ni 50-55, Cr 17-21, Nb+Ta 4.75-5.50 %), a different grain-size and precipitate starting point: the higher solution temperature is the creep-and-ductility route, while the 5596 lower window is the fine-grain tensile route. Both harden on the same double-age cycle afterwards.
5596 vs 5597, the solution temperature is the spec
| AMS 5596 | AMS 5597 | |
|---|---|---|
| Forms | sheet, strip, plate | sheet, strip, plate |
| Solution treatment | 1,700-1,850 °F window | 1,950 °F (1,066 °C) |
| Verified solution-treated sheet condition | 140 ksi UTS / 80 ksi yield / 30 % / ~102 HRB | 140 ksi / 75 ksi yield / 30 % / ≤ 25 HRC |
| After the standard double age | 180 ksi / 150 ksi / 12 % at ≥ 36 HRC | 180 ksi / 150 ksi / 15 % elongation at ≥ 38 HRC |
Read the aged row carefully: same 180/150 strength floors as the 5596 route, but 15 % elongation instead of 12 %: the high-solution route buys transverse ductility and rupture life at equal strength, which is the whole reason the 1,950 °F variant exists.
When the 1,950 °F route wins
The high-solution condition is the tensile-limited-applications alternative: heavy-section parts where transverse ductility and impact strength decide, low-temperature notch-tensile-critical hardware, and creep-rupture-oriented hot-section stock, the same logic that selects AMS 5664 on the bar side of the family. The trade-off the condition tables record is a tendency toward notch brittleness in stress rupture at the coarse-grain extreme, so the selection is duty-driven, not a quality ranking: fine grain (5596 route) for fatigue- and yield-limited sheet parts, 1,950 °F solution (5597 route) for ductility- and rupture-limited duty. The sheet-thickness and gauge page covers the stocked flat-product sizes, the price-by-condition page shows how condition moves the commercial line.
Ordering 5597 sheet correctly
Write the order as: Alloy 718, UNS N07718, sheet per AMS 5597, thickness and width, solution-treated condition (ageing by the buyer where the part is to be aged after forming) or solution-treated-and-aged where the mill runs the cycle, acceptance per AMS 5597 tensile floors, and EN 10204 3.1 with heat chemistry. If the drawing calls the aged condition, require the recorded double-age temperatures (718 °C / 8 h and 621 °C / ≥8 h with the 55 °C/h ramp) on the certificate, the heat-treatment page carries the step table. The RFQ spec writer structures the order lines, the companion AMS 5596 page covers the lower-window document.
How to select the right option for your process
Run the list top to bottom before the enquiry goes out, that is what keeps the part inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
What is AMS 5597?
The SAE aerospace specification for Alloy 718 (UNS N07718) sheet, strip and plate solution treated at 1,950 °F (1,066 °C), the high end of the 718 solution window. After the standard double-age cycle it verifies 180 ksi UTS and 150 ksi yield with 15 % elongation.
AMS 5596 or 5597 for 718 sheet?
Both carry the same chemistry and the same aged strength floors; they differ in solution temperature and what it buys. 5596 (1,700-1,850 °F) is the fine-grain, fatigue-and-yield route; 5597 (1,950 °F) buys transverse ductility and creep-rupture life for tensile-limited heavy-section duty. The drawing decides.
Why does the higher solution temperature add ductility?
A 1,950 °F solution treatment grows the grain and puts more of the strengthening phase into solution before the age. The coarser grain and the redistributed precipitate raise the aged elongation to 15 % versus 12 % on the fine-grain route, at the same 180/150 ksi strength floors.
Does AMS 5597 sheet arrive aged?
The specification covers the solution-treated condition; ageing to the 180 ksi floors happens as a further precipitation heat treatment, run by the mill on request or by the buyer after forming. Require whichever condition the part needs to be stated and recorded on the EN 10204 3.1 certificate.