A nickel-alloy weld is specified in three lines: the parent grade, the AWS A5.14 filler classification, and what happens to the joint afterwards. Most stocked grades take a matching filler whose weld metal mirrors the parent chemistry, a few take an overmatching filler on purpose. Pick the wrong classification and the joint can pass in the coupon and fail in service, the table below pairs every stocked grade with its AWS A5.14 class and the behaviour that class delivers.
Matching filler per stocked grade
Classifications are the AWS A5.14 bare-wire designations (2026 edition), verified against the AWS classification system tables:
| Parent grade | UNS | AWS A5.14 filler | Weld metal character |
|---|---|---|---|
| Inconel 718 | N07718 | ERNiFeCr-2 | precipitation-hardenable, reaches full strength only after the parent’s solution-plus-age cycle |
| Inconel 625 | N06625 | ERNiCrMo-3 | solid-solution Ni-Cr-Mo, usable as-welded, also the overlay and dissimilar-joint workhorse |
| Hastelloy C-276 | N10276 | ERNiCrMo-4 | low-carbon Ni-Cr-Mo-W, no post-weld heat treatment required |
| Hastelloy X | N06002 | ERNiCrMo-2 | oxidation-resistant Ni-Cr-Mo-W for sheet fabrications |
| Incoloy 800 / 800H | N08800 / N08810 | ERNiCr-3 | the standard 80Ni-20Cr wire for furnace and exchanger fabrications |
| Monel 400 / K-500 | N04400 / N05500 | ERNiCu-7 | the Ni-Cu wire across the Monel family, adjusted for weldability |
The classifications and their chemistry windows are defined in AWS A5.14/A5.14M, the parent-grade documents, B637, B443/B444, B575 and the rest, stay on the mill certificate, not on the wire certificate.
The three rules the table hides
Matching is not universal. ERNiFeCr-2 weld metal is designed to age-harden with the parent 718, but as-welded it is nowhere near design strength, so the joint only earns its numbers after the full solution-plus-age cycle. Solid-solution fillers (ERNiCrMo-3, -4) deliver their properties as-welded, which is why 625 and C-276 fabrications rarely see post-weld thermal work. PWHT follows the parent, not the wire. A 718 weld goes through the same double-age cycle as the parent metal, a C-276 weld gets nothing beyond the solution-annealed parent, the grade’s verified feature is weldability without post-weld heat treatment. Dissimilar joints default to the more corrosion-resistant wire. The Ni-Cr-Mo wires bridge nickel alloys to stainless and carbon steels routinely, which is exactly the role ERNiCrMo-3 plays beyond its own 625 repairs.
Ordering wire: the four lines that matter
Write the consumable order as: (1) the AWS classification, ERNiCrMo-4; (2) the form and size, TIG rod or MIG wire, 1.2-2.4 mm typical; (3) the certificate, EN 10204 3.1 with the A5.14 chemistry reported against the classification window; (4) the process note where it matters, cleanliness and interpass control are the failure modes in nickel welding, not the wire itself. The site’s verified pricing on C-276 wire is on the price-per-thickness page (ERNiCrMo-4, 1-5 mm), and the grade-by-grade weldability statements live on the weldability lookup and the weldability hub.
How to select the right option for your process
Five checks, in order. Each one keeps the component inside its specification:
- Step 1: Confirm the maximum service temperature. Fix the peak continuous service temperature the component will see. It decides whether a precipitation-hardened grade such as Inconel 718 (rated 650 °C) or an oxidation-resistant solid-solution grade such as Hastelloy X (rated 1100 °C) is even in the running.
- Step 2: Match the environment and alloy family. Identify the corroding or oxidizing media (chlorides, acids, seawater, combustion gas) and match the family: Ni-Cr-Mo for wet corrosion, Ni-Cu for seawater and hydrofluoric acid, cobalt-base for wear and biocompatibility, precision grades for controlled physical properties.
- Step 3: Choose the product form. Select the semi-finished form: bar and rod (Ø6-350 mm), plate and sheet (0.5-80 mm), strip (0.05-3.0 mm), pipe and tube (OD 6-219 mm), wire (Ø0.10-12.0 mm) or a forged ring, disc or shaft from 5 kg to 3,000 kg.
- Step 4: Set the dimensions and tolerances. State the finished dimensions, condition (hot rolled, cold drawn, solution annealed, spring temper) and surface finish against the form’s stock range, so the mill certificate matches the drawing.
- Step 5: State the standard and certificate. Declare the governing ASTM / AMS / GB/T standard and the certification level: EN 10204 3.1 with heat-specific chemistry, or 3.2 third-party witnessed. The grade is proven by the mill test certificate, not assumed.
Frequently Asked Questions (FAQ)
Which welding wire matches Inconel 718?
ERNiFeCr-2 under AWS A5.14, the precipitation-hardenable 50-55Ni / 17-21Cr / Fe-balance wire whose chemistry mirrors the parent alloy. The weld metal only reaches design strength after the parent 718 solution-plus-double-age cycle, so as-welded joints are interim conditions.
Can I weld C-276 without post-weld heat treatment?
Yes, that is a verified feature of the grade. The low-carbon ERNiCrMo-4 wire and the parent chemistry keep the heat-affected zone out of precipitation territory, so the joint is used as-welded. Where a fabricator chooses to solution anneal, it is a corrosion-uniformity decision, not a strength requirement.
What filler joins Incoloy 800 furnace tubing?
ERNiCr-3, the 80Ni-20Cr classification. It matches the parent 800/800H chemistry closely enough for furnace and exchanger service and is the standard wire behind those fabrications; the joint inherits the parent creep behaviour in the 1100 °C oxidation duty.
Is one filler valid for both Monel 400 and K-500?
ERNiCu-7 covers both, the classification is the Ni-Cu wire across the Monel family. What differs is the joint duty: K-500 joints that must reach the age-hardened strength of the parent need qualification to prove it, since the filler is the weldable adjustment of the 400-family chemistry rather than a strength clone of aged K-500.